Electroless Nickel Plating Cost: How to Quote It per dm²
November 23, 2026
Quote parts like this from a drawing — try it on our sample. Try the sample drawingFree for 30 days · Unlimited quotes · No credit card required
Electroless nickel plating, in Italy nichelatura chimica, deposits a nickel-phosphorus alloy on a part by a chemical reaction in a heated bath, with no electric current. Because there is no current, the layer has the same thickness on flat faces, in bores and in recesses. That is why it is specified for hydraulic blocks, valve bodies, shafts, molds and pump parts that need wear and corrosion resistance, on steel, stainless steel, aluminum or copper alloys.
For a machine shop it is almost always an outside process, and one of the lines most often underpriced in a quote: the plater's price per dm² goes into the estimate, and the thickness it was set for, the bake, the masking, the machining allowance and the minimum lot charge are forgotten. This guide shows how platers price electroless nickel, how thickness, surface and mass relate, and what to add around the plater's invoice. The worked example in EUR prices a batch of steel valve blocks.
How platers price electroless nickel
Platers quote in one of four ways:
- Per dm² (or per m²) of plated surface, at a stated thickness and phosphorus type. Closest to the real cost, because bath time and chemicals scale with surface and thickness.
- Per piece. For small parts, repeat jobs and parts that always hang the same way.
- Per kg. For small parts plated in baskets, where weight stands in for surface.
- Per load. For large parts that fill a tank or need a dedicated bath.
On top come a minimum lot charge, masking of threads, bores and sealing faces that must stay bare, racking for parts that need special fixtures, a charge for extra thickness above the standard, and the bake or hardening heat treatment when the drawing asks for one. Ask for all of them before you quote. The minimum lot charge alone can multiply the price of a small batch.
What drives the price
| Driver | Why it moves the price | Read it on the drawing |
|---|---|---|
| Thickness | Bath time grows with thickness: 50 µm takes twice as long as 25 µm in the same bath | "EN 25 µm" or a minimum thickness |
| Plated surface | Chemicals and tank space scale with area, and bores count | Bores, blind holes, threads |
| Phosphorus type | Low, medium and high phosphorus run in separate baths, so a special type can mean a separate load | "High phosphorus", "non-magnetic", a hardness or corrosion requirement |
| Base material | Steel is plated directly; stainless steel, aluminum and cast iron need extra pre-treatment steps | The material callout |
| Heat treatment | A hydrogen-relief bake for high-strength steel, or hardening of the deposit, is its own operation | "Bake", "heat treat after plating" |
| Masking | Plugs, caps or lacquer on areas that must stay bare | Notes on threads, bores, sealing faces |
| Thickness tolerance | A tight band means more measuring and more rejects | "±5 µm" |
| Documents | Thickness report, adhesion test, certificate | Notes and the purchase order |
Electroless nickel follows the surface it is plated on, so the finish before plating sets the finish after.
Thickness, surface and mass
Three conversions cover most of what an estimator needs:
- deposit mass per dm² (g) = thickness (µm) × density (g/cm³) ÷ 100
- plating time (h) = thickness (µm) ÷ deposition rate (µm/h)
- every plated surface grows by the thickness: a shaft diameter by 2 × thickness, a bore shrinks by 2 × thickness
The table assumes a density of 8.0 g/cm³ and a deposition rate of 10 µm/h. Both are assumptions: ask the plater for the figures of the bath.
| Thickness | Deposit mass | Plating time | Diameter change |
|---|---|---|---|
| 5 µm | 0.40 g/dm² | 0.5 h | 10 µm |
| 12 µm | 0.96 g/dm² | 1.2 h | 24 µm |
| 25 µm | 2.00 g/dm² | 2.5 h | 50 µm |
| 50 µm | 4.00 g/dm² | 5.0 h | 100 µm |
| 75 µm | 6.00 g/dm² | 7.5 h | 150 µm |
The last column reaches the machining. An h7 fit on Ø30 is 21 µm wide, and 25 µm of deposit changes the diameter by 50 µm: the part has to be machined undersize by that amount, with the deposit held tighter than the fit, or ground after plating.
A price per kg is fair only for parts with the same surface per kg: for sheet it is 2 ÷ (density × thickness), for round bar 4 ÷ (density × diameter). Steel at 7,850 kg/m³ gives 12.74 dm²/kg for 2 mm sheet and 1.02 dm²/kg for Ø50 bar. At an assumed €0.60/dm², €0.61 per kg suits the bar; the same plating on the sheet costs €7.64 per kg, 12.5 times more.
The costs around the plater's price
| Line | What it covers |
|---|---|
| Plater's price | Per dm², per piece or per kg at the stated thickness, at least the minimum lot charge |
| Masking | Plugs, caps or lacquer for threads, bores and sealing faces |
| Bake or hardening | Hydrogen-relief bake or hardening heat treatment, usually its own line |
| Machining allowance | Parts machined undersize by twice the deposit, or ground after plating |
| Your uplift | Risk of rejects, capital tied up, the plater's lead time |
| Transport | Both ways, per batch |
| Preparation and packing | Parts clean of oil and chips, counted, packed so the deposit is not scratched |
| Receiving inspection | Thickness on a sample, adhesion, visual check, fit of critical diameters |
A plated thread is tighter, so mask it or cut it with the deposit in mind. If the drawing only asks for a light protective or decorative layer, electrolytic nickel is priced differently; for a hard wear layer the other usual candidate is hard chrome. A bake or hardening step is quoted like any other heat treatment.
Worked example: 150 steel valve blocks
150 valve blocks in steel, 100 × 60 × 40 mm, with 25 µm of medium-phosphorus electroless nickel. The two Ø16 threaded ports are plugged to keep the threads bare, so only the outer faces are plated: 2 × (100 × 60 + 100 × 40 + 60 × 40) = 24,800 mm², or 2.48 dm² per block. The figures are example figures, not market prices: the plater charges €0.60/dm² at 25 µm with a €150 minimum lot charge and €0.30 per masking plug; transport is €55 each way; your preparation and packing take 0.8 minutes per part at €45/h; receiving inspection takes 1.5 hours at €55/h; your uplift on the plater's invoice is 10%.
| Line | Calculation | Cost |
|---|---|---|
| Plating | 150 × 2.48 dm² × €0.60/dm² | €223.20 |
| Masking | 150 × 2 plugs × €0.30 | €90.00 |
| Plater's invoice (above the minimum) | €223.20 + €90.00 | €313.20 |
| Uplift | 10% of €313.20 | €31.32 |
| Transport | 2 × €55 | €110.00 |
| Preparation and packing | 150 × 0.8 min × €45/h | €90.00 |
| Receiving inspection | 1.5 h × €55/h | €82.50 |
| Total | €627.02 |
That is €4.18 per block. The plating price alone was €1.49 per block: an estimate that used only that number would have covered about a third of the real cost of the line.
On a batch of 15 blocks the plating and masking come to €31.32, below the €150 minimum lot charge, so the plater invoices €150.00. The uplift becomes €15.00 and preparation and packing €9.00; with transport and inspection unchanged the total is €366.50: €24.43 per block. For small batches the minimum lot charge is the price, and it is worth asking whether the blocks can ride with another customer's load.
FAQ: electroless nickel plating cost
How is electroless nickel plating priced? Platers quote per dm² of plated surface at a stated thickness, per piece, per kg for small parts, or per load, plus a minimum lot charge and masking. Per dm² follows the plater's real cost best, because bath time and chemicals scale with surface and thickness.
How does thickness change the cost of electroless nickel? Plating time grows in proportion to thickness: at an assumed 10 µm/h, 25 µm takes 2.5 hours and 50 µm takes 5.0 hours. A thicker deposit also changes diameters and widths by twice its thickness, so the machining of the part has to change with it.
How do you convert an electroless nickel price per kg into a price per dm²? Divide the price per kg by the surface per kg of the part. For 2 mm steel sheet the surface per kg is 12.74 dm², for Ø50 steel bar 1.02 dm². A price per kg is therefore fair only for parts of similar shape and size.
Why does plating a small batch cost so much per part? Because of the minimum lot charge, transport and inspection, which are paid per batch. In the example in this article 150 blocks cost €4.18 each and 15 blocks cost €24.43 each, although the price per dm² is the same.
Electroless nickel plating in QuoteBuddy
QuoteBuddy reads the technical drawing, including the notes, and builds the estimate as separate lines at your own rates. A plating called out on the drawing becomes its own coating operation, and a bake or hardening treatment becomes its own heat-treatment operation. QuoteBuddy does not tell electroless nickel apart from other platings, so the line is priced at the rate you set. When plating is not one of your in-house capabilities, it is treated as outsourced: priced with your outsourcing uplift, with an outsourcing handling line once per order, and flagged for review until you confirm the step and enter the supplier's hourly rate. The setup minutes, cycle minutes and hourly rate of an operation line can be edited, so the line can match the plater's real price. See also make or buy for the cost of any outside operation.
You can watch the QuoteBuddy demo video, from technical drawing to quote. To try it on a drawing of your own, start a free 30-day trial.